52100轴承钢
钼 Mo:≤0.08
52100轴承钢热处理
其热处理制度为:钢棒退火,钢丝退火或830-840度油淬。 热处理工艺参数: 1.普通退火:790-810度加热,炉冷至650度后,空冷——HB170-207 2.等温退火:790-810度加热,710-720度等温,空冷——HB207-229 3.正 火:900-920度加热,空冷——HB270-390 4.高温回火:650-700度加热,空冷——HB229-285 5.淬 火:860度加热,油淬——HRC62-66 6.低温回火:150-170度回火,空冷——HRC61-66 7.碳氮共渗:820-830度共渗1.5-3小时,油淬,-60度至-70度深冷处理 +150度至+160回火,空冷——HRC≈67。
常用日本铬钢牌号: SCR415 SCR420 SCR430 SCR435 SCR440 SRC445等
常用铬钼合金结构钢:SCM415 SCM418 SCM420 SCM430 SCM435 SCM440等
20Cr,5120,SCr420,35Cr,SCr435,37Cr4,5135,40Cr,SCr440,41Cr4,5140,15CrMo,SCM415,13CrMo4-5,20CrMo,SCM418,18CrMo4,25CrMo4,20CrMnMo,20MnCr5,35CrMo,SCM435,4137,34CrMo4,1.7220,35CrMoV,31CrMoV9,42CrMo,SCM440,4170,42CrMo4,1.7225,4140,40CrMnMo,42CrMoA,38CrMoAL,SACM645,41CrALMo7,1.8509,20CrMnTi,40CrNIMoA,SNCM432,4340,36CrNiMo4,1.6511,40CrH,4130,16Mn,T10,30CrMo,SCM430,16MnCr5,16MnCr5H,SMnC420,5120H,17CrNiMo6,34CrNiMo6,18CrNiMo7-6,50CrVA,SUP10,SUP9,6150,51CrV4,1.8759,60Si2Mn,65Mn,1065,1050,1070,9260,61SiCr7,1.7108,60Si2MnA,50CrV4,SK3,SK4,SK5,SK7,SUJ2,GCr15,52100,100Cr6,9Cr18MoV,SUS440C,GCr15SiMo,GCr15SiMn
52100轴承钢价格 52100轴承钢性能
52100钢材是一种最常用的高铬轴承钢,具有高的淬透性,热处理后可获得高而均匀的硬度。耐磨性优于GCr15,接触疲劳强度高,有良好的尺寸稳定性和抗蚀性,冷变形塑性中等,切削性一般,焊接性差,对白点形成敏感,有第一类回火脆性。 在滚珠轴承制造中,用以杂质壁厚12mm.外径<250mm的H级至C级的轴承套,直径25.4-50.8mm的钢球;直径<22mm的滚子,此外也可用作承受大负荷.要求高耐磨性.高弹性极限.高接触疲劳强度的其他机械零件及各种精密量具冷冲模等。如机床的滚珠丝杆,涡轮喷气发动机喷嘴的喷口.柱塞.活门.衬套等。
52100轴承钢化学成份:
碳 C :0.95~1.05
硅 Si:0.17~0.37
锰 Mn:0.20~0.40
硫 S :≤0.020
磷 P :≤0.027
铬 Cr:1.30~1.65
镍 Ni:≤0.30
铜 Cu:≤0.25
52100轴承钢力学性能:
抗拉强度 σb (MPa):1617
冲击功 Akv (J):28
硬度 :61~64HRC
试样尺寸:某试样
热处理规范及金相组织:
热处理规范:850~860℃淬火,油冷;160℃回火2h。
金相组织:回火马氏体。
交货状态:以热轧(锻制)退火,不退火,退火剥皮钢,冷拉(轧)圆钢,磨光圆钢,热轧钢管,退火剥皮钢管,冷拉(轧)钢管八种状态交货。
4720h 4817h 4820h 5120h 8617h 8620h 9310h 3310 4320 4620 4720 4820 52100 52100Mod.1
52100Mod.2 52100Mod.3 52100Mod.4 8620 9310 440c 440cMod 1030 1040 1050 1541 1552 4130 4140
5140 5150 6150 SNCM220 SSNCM240 SCNM415 SNCM415 SNCM420 SNCM431 SNCM439 SNCM447
SNCM616 SNCM625 SNCM630 SNCM815 GCr9 51100 SUJ1 GCr15 52100 SUJ2 100Cr6 9Cr18Mo 440C SUS440C Z100CD17 等